Sep 27 2012
Phosphorus-deoxidized UNS C12500 has a copper content of not less than 99.88%.
The following table outlines the mechanical properties of UNS C12500 wires as a function of heat treatment and thickness.
Temper |
Thickness |
Tensile Str. |
Elong. |
Shear Str. |
H04 |
2 mm (0.08 in) |
379 MPa (55 ksi) |
1% |
200 MPa (29 ksi) |
H08 |
2 mm (0.08 in) |
455 MPa (66 ksi) |
1% |
228 MPa (33 ksi) |
OS050 |
2 mm (0.08 in) |
241 MPa (35 ksi) |
35% |
165 MPa (24 ksi) |