Copper UNS C19100 has a copper content of not less than 98.2%.
The following table shows the mechanical properties of UNS C19100 rods as a function of heat treatment and thickness.
Temper |
Thickness |
Tensile Str. |
Yield Str. |
Elong. |
Rockwell |
Shear Str |
Fatigue Str. |
B |
C |
F |
30T |
HR01 |
9.53mm (0.375in) |
648MPa (94ksi) |
517MPa (75ksi) |
10% |
90 |
- |
- |
- |
331MPa (48ksi) |
- |
|
12.7mm (0.5in) |
552MPa (80ksi) |
483MPa (70ksi) |
15% |
85 |
- |
- |
- |
296MPa (43ksi) |
- |
|
25.4mm (1in) |
538MPa (78ksi) |
469MPa (68ksi) |
27% |
84 |
- |
- |
- |
283MPa (41ksi) |
228MPa (33ksi) |
The chemical composition of UNS C19100 copper alloy is outlined in the following table.
Element |
Content (%) |
Nickel, Ni |
0.9-1.3 |
Tellurium, Te |
0.35-0.6 |
Iron, Fe |
0.2 |
Phosphorous, P |
0.15-0.35 |
Lead, Pb |
0.1 |
Zinc, Zn |
0.5 |
Copper, Cu |
Remainder |