Sep 27 2012
UNS C18200 chromium copper alloy has a copper content of not less than 99.1%.
The following table outlines the mechanical properties of UNS C18200 flat products as a function of heat treatment and thickness.
Temper |
Thickness |
Tensile Str. |
Yield Str. |
Elong. |
Rockwell |
B |
C |
F |
30T |
TB00 |
1 mm (0.04 in) |
234 MPa (34 ksi) |
131 MPa (19 ksi) |
40% |
16 |
- |
- |
- |
TF00 |
1 mm (0.04 in) |
352 MPa (51 ksi) |
248 MPa (36 ksi) |
22% |
59 |
- |
- |
- |
TH01 |
1 mm (0.04 in) |
462 MPa (67 ksi) |
407 MPa (59 ksi) |
14% |
79 |
- |
- |
- |
Equivalent materials to UNS C18200 copper alloy are: