UNS C40860 has a copper content of not less than 94%.
Tabulated below are the mechanical properties of UNS C40860 flat products as a function of heat treatment and thickness.
Temper |
Tensile Str. |
Elong. |
H01 |
408MPa (59ksi) |
24% |
H02 |
441MPa (64ksi) |
12% |
H04 |
552MPa (80ksi) |
6% |
H08 |
662MPa (96ksi) |
3% |
H06 |
634MPa (92ksi) |
4% |
OS015 |
365MPa (53ksi) |
42% |
The chemical composition of UNS C40860 copper alloy is outlined in the following table.
Elements |
Content (%) |
Copper, Cu |
94.0-96.0 |
Tin, Sn |
1.7-2.3 |
Nickel, Ni |
0.05-0.20 |
Lead, Pb |
0.05 |
Phosphorus, P |
0.02-0.04 |
Iron, Fe |
0.01-0.05 |
Zinc, Zn |
Remainder |