Nov 29 2012
UNS C42500 has a copper content of not less than 87%.
Tabulated below are the mechanical properties of UNS C42500 flat products as a function of heat treatment and thickness.
Temper |
Thickness |
Tensile Str. |
Yield Str. |
Elong. |
Rockwell |
B |
C |
F |
30T |
H01 |
1mm (0.04 in) |
372MPa (54ksi) |
193MPa (45ksi) |
35% |
60 |
- |
- |
56 |
H02 |
1mm (0.04 in) |
43MPa (63ksi) |
345MPa (50ksi) |
20% |
75 |
- |
- |
68 |
H03 |
1mm (0.04 in) |
469MPa (68ksi) |
393MPa (57ksi) |
15% |
80 |
- |
- |
70 |
H04 |
1mm (0.04 in) |
524MPa (76ksi) |
434MPa (63ksi) |
95 |
86 |
- |
- |
73 |
H06 |
1mm (0.04 in) |
565MPa (82ksi) |
483MPa (70ksi) |
7% |
90 |
- |
- |
74 |
H08 |
1mm (0.04 in) |
614MPa (89ksi) |
517MPa (75ksi) |
4% |
92 |
- |
- |
76 |
H10 |
1mm (0.04 in) |
634MP (92ksi) |
524MPa (76KSI) |
2% |
92 |
- |
- |
76 |
OS015 |
1mm (0.04 in) |
324MPa (47ksi) |
138MPa (20ksi) |
47% |
- |
- |
79 |
45 |
OS025 |
1mm (0.04 in) |
317MPa (46ksi) |
124MPa (18ksi) |
48% |
- |
- |
72 |
36 |
OS035 |
1mm (0.04 in) |
310MPa (45ksi) |
124MPa (18ksi) |
49% |
- |
- |
70 |
32 |
The chemical composition of UNS C42500 copper alloy is outlined in the following table.
Elements |
Content (%) |
Copper, Cu |
87.0-90.0 |
Tin, Sn |
1.5-3.0 |
phosphorus, P |
0.35 |
Iron, Fe |
0.05 |
Lead, Pb |
0.05 |
Zinc, Zn |
Remainder |
Equivalent material to UNS C42500 copper alloy includes ASTM B591.