Dec 10 2012
UNS C65100 low-silicon bronze B has a copper content of not less than 98.5%.
The following table shows the mechanical properties of UNS C65100 rods as a function of heat treatment and thickness.
Temper |
Thickness |
Tensile Str. |
Yield Str. |
Elong. |
Rockwell |
B |
C |
F |
30T |
OS035 |
25.4 mm (1 in) |
276 MPa (40 ksi) |
103 MPa (15 ksi) |
50% |
- |
- |
55 |
- |
The chemical composition of UNS C65100 copper alloy is outlined in the following table.
Element |
Content (%) |
Zinc, Zn |
1.5 |
Silicon, Si |
0.8-2.0 |
Iron, Fe |
0.8 |
Manganese, Mn |
0.7 |
Lead, Pb |
0.05 |
Copper, Cu |
Remainder |
Equivalent materials to UNS C65100 copper alloy are:
-
ASME SB315
-
ASME SB98
-
ASTM B105
-
ASTM B315
-
ASTM B432
-
ASTM B96
-
ASTM B98
-
ASTM B99
-
ASTM F467
-
ASTM F468