Nov 29 2012
UNS C67400 has a copper content of not less than 57%.
The following table shows the mechanical properties of UNS C67400 rods as a function of heat treatment.
Temper |
Thickness |
Tensile Str. |
Yield Str. |
Elong. |
Rockwell |
Shear Str. |
Fatigue Str. |
B |
C |
F |
30T |
HR02 |
19 mm. (0.75 in.) |
634MPa (92ksi) |
379MPa (55ksi) |
20% |
87 |
- |
- |
- |
331MPa (48ksi) |
200MPa (29ksi) |
O60 |
19 mm. (0.75 in.) |
483MPa (70ksi) |
234MPa (34ksi) |
28% |
78 |
- |
- |
- |
- |
- |
Equivalent materials to UNS C67400 copper alloy are given below:
The chemical composition of UNS C67400 copper alloy is outlined in the following table.
Element |
Content (%) |
Copper, Cu |
57-60 |
Manganese, Mn |
2.0-3.5 |
Aluminum, Al |
0.50-2.0 |
Silicon, Si |
0.50-1.5 |
Lead, Pb |
0.5 |
Iron, Fe |
0.35 |
Tin, Sn |
0.3 |
Nickel, Ni |
0.25 |
Zinc, Zn |
Remainder |