Copper UNS C93200 has a copper content of not less than 81%.
The following table shows the mechanical properties of UNS C93200 sand cast alloy as a function of heat treatment.
Temper |
Tensile Str. |
Yield Str. |
Elong. |
Fatigue Str. |
M01 |
207MPa (30ksi) |
97MPa (14ksi) |
15% |
- |
|
241MPa (35ksi) |
124MPa (18ksi) |
20% |
110MPa (16ksi) |
Equivalent materials to UNS C93200 copper alloy are the following:
- ASTM B271
- ASTM B30
- ASTM B505
- ASTM B584
- ASTM B763
- QQ C390
- SAE 660
- SAE J461
- SAE J462
The chemical composition of UNS C93200 copper alloy is outlined in the following table.
Element |
Content (%) |
Copper, Cu |
81-85 |
Tin, Sn |
6.3-7.5 |
Lead, Pb |
6-8 |
Zinc, Zn |
1-4 |
Nickel, Ni |
1 |
Antimony, Sb |
0.35 |
Iron, Fe |
0.2 |
Phosphorous, P |
0.15 |
Sulfur, S |
0.08 |
Silicon, Si |
0.005 |
Aluminum, Al |
0.005 |