Nov 29 2012
UNS C42600 has a copper content of not less than 87%.
Tabulated below are the mechanical properties of UNS C42600 flat products as a function of heat treatment.
Temper |
Tensile Str. |
Elong. |
H01 |
469MPa (68ksi) |
- |
|
- |
20% |
H02 |
- |
10% |
|
552MPa (80ksi) |
- |
H04 |
- |
6% |
|
634MPa (92ksi) |
- |
H06 |
- |
4% |
|
724MPa (105ksi) |
- |
H08 |
793MPa (115ksi) |
- |
|
- |
2% |
H10 |
- |
1% |
|
834MPa (121ksi) |
- |
OS015 |
414MPa (60ksi) |
- |
|
- |
35% |
The chemical composition of UNS C42600 copper alloy is outlined in the following table.
Elements |
Content (%) |
Copper, Cu |
87.0-90.0 |
Tin, Sn |
2.5-4.0 |
Iron, Fe |
0.05-0.20 |
Nickel, Ni |
0.05-0.20 |
Lead, Pb |
0.05 |
Phosphorus, P |
0.01-0.20 |
Zinc, Zn |